Experimental Studies of Failure Behavior and Strength of H Beams with Stiffened Web Openings under Compression and Bending Loads

2016-05-16 02:42:03,,
船舶力學 2016年3期
關鍵詞:承載力船舶研究

,,

(1 Key Laboratory of High Performance Ship Technology of Ministry of Education,Wuhan University of Technology, Wuhan 430063,China;2 China Ship Development and Design Center,Wuhan 430064,China)

Experimental Studies of Failure Behavior and Strength of H Beams with Stiffened Web Openings under Compression and Bending Loads

ZHAO Ying-jiang1,YAN Ren-jun1,WANG Hong-xu2

(1 Key Laboratory of High Performance Ship Technology of Ministry of Education,Wuhan University of Technology, Wuhan 430063,China;2 China Ship Development and Design Center,Wuhan 430064,China)

Steel H beams with web openings are widely used as flexural members in ships,aircrafts, and offshore structures.In spite of numerous papers in the literature on beams with web openings subjected to web crippling,the effect of stiffened web openings subjected to plate buckling has not been exhaustively examined.Hence a detailed experiment study involving six specimens was undertaken to investigate the failure behavior and ultimate capacity load of H beams with stiffened web openings. The results show that the wavelength and quantities of the buckling waves were modified by the hole.This study can be used in practical structures with similar geometric features.

H beams;web openings;buckling waves;failure behavior; ultimate capacity load

0 Introduction

Opening H beams are used to lighten the ship,aircraft and make a way of access for air, pipeline or cable in ship and offshore structures.The presence of the openings(perforations) will cause structural discontinuity,stress redistribution and declining of ultimate bearing capacity.The girders and beams in ship and offshore structures are usually subjected to longitudinal thrust and vertical pressure.Under such combined loads,the behavior of the opening H beams is hard to be realized and the influence of related parameters become complex.

Thin plates with holes,which were primarily motivated by the design needs of the aerospace industry in early studies[1-2].Critical load was reduced and axial force in the plate strips adjacent to the hole was concentrated due to the existence of hole.Further study extended to beam with web openings[3-4].The parameters such as hole sizes,positions and shapes influencing the web crippling behaviors of opening beams are discussed and analysized.It is interesting that the presence of hole can either decrease or increase the critical elastic buckling stress andchange the length and quantity of buckled half-waves[5-6].

It is worth mentioning here that all the relevant researches above on H beams are subjected to web crippling behaviors.It is only one of typical collapse patterns that are classified into six groups by Paik[7],the collapse of the stiffened panel occurs at the lowest value among the various ultimate load calculated for each of the collapse patterns.In these situations,an appropriate cutout strengthening method is adopted to improve the ultimate load of H beams. Hence,H beams can avoid web crippling if the stiffeners are strong enough.However,the kind of experiment has not been carried out until now.Herein,in this paper,the detail failure behavior of H beams with stiffened web openings is investigated.On the basis of changing the hole positions we will explain the influence on failure behavior of H beams subjected to buckling or collapse of plate.

1 Strength experiment

In order to provide sufficient stiffness and to avoid web crippling,the basic geometry and notations of the specimens are shown in Fig.1.The specimens are composed of plating(333 mm× 10 mm×3 000 mm),stiffener web(240 mm×6 mm×3 000 mm)and stiffener flange(80 mm× 8 mm×3 000 mm).Location of the hole in stiffener web can be seen in Tab.1.The specimens are divided into series 1 and series 2 based on the location of the hole(see Tab.1).The behavior of the H beams subjected to compression and bending loads were observed.

Fig.1 Dimensions of the specimen

1.1 Specimen and equipment

The test specimens were fabricated using hot-rolled steel plating of Q235 which were most commonly used in ship hull building.The plates were cut by CNC plasma cutting technology.Weld uses manual arc welding,and the corresponding welding material is V840 electrode.One week was allowed for cooling in order to minimize the effect of initial distortion caused by excessive heating and to keep the residual stress minimum.

Tab.1 Hole location

To analyze the limit behavior of opening H beams subjected to compression and bending loads,an original experiment setup has been developed.An overview of the test rig is shown in Fig.2.Longitudinal thrust was controlled by MTS electro-hydraulic actuator with a capacity of 500 kN,the electro-hydraulic actuator could transfer hydraulic energy to mechanic energy and control the load accurately with a displacement sensor inside.Compression load was applied to the neutral axis of the specimen.In the vertical direction,bending load was simulated by five concentrated forces which were provided by hydraulic jacks with a capacity of 200 kN for everyone.Low carbon steel circular shafts were introduced at both end of the specimen and reaction frame to constraint the displacement and allow rotation of the end of the specimen. The electronic dial indicator was set to monitor the deflection of the middle of the specimen and strain gauges to monitor the strains of the specimen in the process of loading.A sectional view of the testing rig showing the details of load application is given in Fig.2.

The existence of the opening would result in the stress concentration of the plates near the hole,the stress level near the hole would reach the yield stress quickly.To improve the local buckling of the specimen of the perforated plates,we can adopt an appropriate cutoutstrengthening method and welding progress from Paik[7].The strengthening stiffener combined two parts,one was a plate with thickness of 6 mm and width of 300 mm is symmetrically welded to the perforated plate at their circular intersections after being rolled into a ring,another was a rectangular flat plate with a slotted hole that has the same size of the opening in the web,the plate was welded to the web with two circles being concentric.The welding is finally carried out along the inner edge and the four outer edges of the flat stiffener.

Fig.2 Overall and detail view of the test rig

1.2 Test procedure

All specimens were tested with two ends simply supported on the reaction frame.Before testing,the specimen should be positioned accurately to guarantee both compression load and neutral axial collinear.To ensure the safety and running well of the test,a small load of compres-sion load and bending load was applied and released before formal loading,respectively.Observe whether the instrument reading is in the normal level.

Compression load were applied to the neutral axial of the specimen firstly.Load level increased to 450 kN and with the compression load maintained constant at this level,the specimen wsa tested to failure by gradually increasing the vertical pressure.Reading of the electronic dial indicator and strain gauges were recorded for each increment of load.Buckling behavior of the specimen could be analyzed from the load-deflection curve or the load-strain curve obtained from the computer output.

2 Test results and discussions

2.1 Observations

As mentioned above,an appropriate cutout-strengthening method and welding progress were taken to avoid web crippling and improve the bulking capacity of the specimens.The buckling or collapse behavior of web did not occur in the test process.The results of failure modes of the specimens are shown in Fig.3 and Fig.4.As can be seen in Tab.1,BG-4,BG-5, and BG-6 were the specimens with hole at the edge of the web.For these specimens,similar buckling initiated at the mid-span of the plate.The initial buckling was followed by global buckling and the local buckling waves deepened at the same time.Fig.3 shows the specimens with hole at the mid-span of the specimens.As it is shown by red arrows in Fig.3,for BG-1 double buckling lobes occurred at the plate close to both sides of web opening,one buckling lobe occurred at the plate close to one side of web opening in BG-2,one buckling lobe occurred at the plate just below web opening in BG-3.

Fig.3 Failure mode of test specimens(a)BG-1;(b)BG-2;(c)BG-3;(d)BG-4;(e)BG-5;(f)BG-6

The following observations can be highlighted based on the above curves:

(1)The previous research[8-9]has indicated that the global buckling mode and local buck-ling mode are sensitive to the position of holes and local buckling mostly occurred at zone adjacent to hole.However,due to the stiffened structure of the web opening,the influence to the failure mode are local buckling modes of the plate other than global buckling modes of the specimens.

(2)For specimens with stiffened web opening at the edge of the web,the local buckling modes were similar with each other.

(3)For specimens with stiffened web opening at the mid-length of the web,as the vertical position of web opening varied,quantities and half wavelength of local buckling lobes were different.

2.2 Load capacity of the specimens

As mentioned earlier,the present specimens were subjected to compression and bending loads.The variation of vertical mid-span displacement is incredibly small in the step one(less than 1 mm).In each of these figures,only the vertical loads and the corresponding vertical displacement are plotted.Experimentally obtained load-displacement curves for series 1 and series 2 are summarized in Figs.4 and 5,respectively.

It is obviours that the ultimate capacity of specimens in series 2 are approximately in the same level of 365 kN,failure occurred around 97%,101%and 105%of the ultimate capacity of specimens in series 2 for specimen BG-1,BG-2 and BG-3 respectively,the effects were smaller than specimens subjected to web crippling.Combined with the corresponding failure mode in Fig.2 and Fig.3,we believe that the local buckling wave mode of the plate is directly related to the ultimare capacity of H beams.

Fig.4 Load-displacement curves for series 1

Fig.5 Load-displacement curves for series 2

As to the similar specimens in Konstantinos[10],a significant and sudden drop of load occurred directly after reaching the ultimate load capacity.This phenomenon did not occur in the experiment process,the reason is that the collapse patterns have been changed due to the existence of the stiffened web openings that can avoid web crippling behavior.

3 Conclusions

The present paper summarizes detail phenomena of six H beams with stiffened web open-ings in order to extract the relationship between the buckling wave modes of the plates and ultimate capacity loads under compression and bending loads.The results of the current study can be summarized as follows:

(1)The cutout-strengthening method and welding progress in this paper can avoid web crippling effectively.The failure behavior begins from the local buckling of the plate in the mid-span of the specimen.

(2)The local buckling wave modes of the plates were quite dependent on the opening location especially when opening locating at the adjacent region of the buckling wave.

(3)The local buckling wave modes have an important impact on the ultimate capacity loads.

(4)More work needs to be done in this research field to explore the relationship between the buckling wave modes of the plates and ultimate capacity loads under compression and bending loads.

Acknowledgements

The authors would like to thank Mr.Jun Ke and Geng Xu and Ms Jing Lin from Wuhan U-niversity of Technology for their help.

[1]Schlack Jr AL.Elastic stability of pierced square plates[J].Experimental Mechanics,1964,4(6):167-72.

[2]Rhodes J,Nash D.An investigation of web crushing behavior in thin-walled beams[J].Thin-Walled Structures,1998:207-230.

[3]Mahendran M,Keerthan P.Experimental studies of the shear behavior and strength of LiteSteel beams with stiffened web openings[J].Engineering Structures,2013:840-854.

[4]Keerthan P,Mahendran M.Experimental studies of the shear behavior and strength of lipped channel beams with web openings[J].Thin-Walled Structures,2013:131-144.

[5]Moen C D,Schafer B W.Elastic buckling of thin plates with holes in compression or bending[J].Thin-Walled Structures, 2009:1597-1607.

[6]Moen C D,Schafer B W.Elastic buckling of cold-formed steel columns and beams with holes[J].Engineering Structures, 2009:2812-2824.

[7]Jeom Kee Paik,Bong Ju Kim.Ultimate strength formulations for stiffened anels under combined axial load,in-plane ending and vertical pressure:A benchmark study[J].Thin-Walled Structures,2002,40:45-83.

[8]Ellobody E.Interaction of buckling modes in castellated steel beams[J].Journal of Constructional Steel Research,2011: 814-825.

[9]El-Sawy K M,Nazm A S.Effect of aspect ratio on the elastic buckling of uniaxially loaded plates with eccentric holes[J]. Thin-Walled Structures,2001:983-998.

[10]Tsavdaridis K Daniel,D’Mello C,Huo Bingyu.Experimental and computational study of the vertical shear behavior of partially encased perforated steel beams[J].Engineering Structures,2013:805-822.

腹板開孔的H型梁在壓彎載荷下的失效行為和強度試驗研究

趙應江1,嚴仁軍1,王紅旭2

(1武漢理工大學 高速船舶工程教育部重點實驗室,武漢 430063;2中國艦船研究中心,武漢430064)

腹板開孔的H型鋼梁在船舶,航空器和海洋平臺結構作為受彎構件被廣泛運用。已有眾多文獻報道過關于腹板開孔梁遭受腹板卷曲破壞的情況,但腹板開孔加強遭受面板屈曲的情況未有詳盡調查。因此文中開展6組試件的試驗研究來調查腹板開孔的H型梁的失效行為和極限承載力,結果顯示開孔影響了試件屈曲波的長度和數量。該研究結果可用于幾何尺寸相似的實際結構。

H型梁;腹板開孔;屈曲波;失效行為;極限承載力

U661.72

:A

趙應江(1989-),男,武漢理工大學交通學院博士研究生;

U661.72

A

10.3969/j.issn.1007-7294.2016.03.008

1007-7294(2016)03-0315-08

嚴仁軍(1962-),男,武漢理工大學交通學院教授/博士生導師。

Received date:2015-09-21

Foundation item:Supported by Fundamental Research Funds for the Central Universities(WUT:2016IVA009)

Biography:ZHAO Ying-jiang(1989-),male,Ph.D.student of Wuhan University of Technology,E-mail:

zhao_yingjiang@163.com;YAN Ren-jun(1962-),male,professor/tutor.

猜你喜歡
承載力船舶研究
計算流體力學在船舶操縱運動仿真中的應用
FMS與YBT相關性的實證研究
《船舶》2022 年度征訂啟事
船舶(2021年4期)2021-09-07 17:32:22
遼代千人邑研究述論
船舶!請加速
視錯覺在平面設計中的應用與研究
科技傳播(2019年22期)2020-01-14 03:06:54
EMA伺服控制系統研究
CFRP-PCP板加固混凝土梁的抗彎承載力研究
耐火鋼圓鋼管混凝土柱耐火極限和承載力
潛艇極限承載力計算與分析
主站蜘蛛池模板: 亚洲欧美激情小说另类| 99久久这里只精品麻豆| 在线观看无码av免费不卡网站 | 尤物特级无码毛片免费| 找国产毛片看| 国产91高跟丝袜| 三区在线视频| 国产精品成人免费综合| a级毛片免费看| 国产在线观看人成激情视频| 全部免费毛片免费播放| 日本亚洲国产一区二区三区| 天堂av高清一区二区三区| 在线免费亚洲无码视频| 国产精品极品美女自在线| 中文字幕第1页在线播| 人人爽人人爽人人片| 免费国产一级 片内射老| 成年女人a毛片免费视频| 狼友av永久网站免费观看| 国产精品成人啪精品视频| 欧美亚洲一区二区三区在线| 特级精品毛片免费观看| 在线观看免费国产| 22sihu国产精品视频影视资讯| 又黄又湿又爽的视频| 中文字幕永久在线看| 久久久久国产精品嫩草影院| 色成人综合| 日本三区视频| 亚洲成人高清无码| 国产日本欧美亚洲精品视| 毛片免费在线视频| 亚洲色精品国产一区二区三区| 久久精品亚洲中文字幕乱码| 国产精品蜜臀| 99精品国产电影| 亚洲成人动漫在线| 亚洲精品无码抽插日韩| 中文成人在线视频| 97人人做人人爽香蕉精品| 婷婷综合在线观看丁香| 色综合天天娱乐综合网| 国产理论最新国产精品视频| 国产不卡网| 国产精女同一区二区三区久| 尤物亚洲最大AV无码网站| 国产精品香蕉在线观看不卡| 日韩福利在线视频| 992tv国产人成在线观看| 国产精品专区第1页| 91国语视频| 国产成人资源| 永久免费AⅤ无码网站在线观看| 狠狠色狠狠综合久久| 欧美日韩资源| 精品偷拍一区二区| 91国内在线观看| 国产香蕉一区二区在线网站| 永久在线精品免费视频观看| 午夜视频在线观看区二区| 99在线视频免费观看| 99精品福利视频| 青青草国产在线视频| 免费毛片视频| 亚洲国产天堂久久综合226114| 国产成人a毛片在线| 亚卅精品无码久久毛片乌克兰| 67194亚洲无码| 亚洲国产成人精品无码区性色| 色噜噜狠狠色综合网图区| lhav亚洲精品| 精品国产成人三级在线观看| 欧洲欧美人成免费全部视频 | 国产免费久久精品99re丫丫一| 中文字幕66页| 国产一区二区三区在线观看视频| 国产va在线观看免费| 国内精自视频品线一二区| 无码又爽又刺激的高潮视频| 久久久噜噜噜| 国产午夜在线观看视频|