Effect of PSA tin plating process on trace lead in tin coating☆

2015-11-01 07:35:38BinghuLiKuaikuaiGuoChangshengLiu
Chinese Journal of Chemical Engineering 2015年10期

Binghu Li,Kuaikuai Guo ,Changsheng Liu ,*

1 Key Laboratory for Anisotropy and Texture of Materials of Ministry of Education,Northeastern University,Shenyang 110819,China

2 Baoshan Iron&Steel Group,Shanghai 201900,China

Keywords:Optimal design Process control Safety Tin plating Trace Pb Current density Bath temperature

ABSTRACT In this paper,effects of conditions in phenol sulfonic acid(PSA)plating for tin coating of MR low carbon aluminum killed steel on trace Pb were examined.Trace Pb was measured by atomic absorption spectrometry(AAS)and glow discharge spectrometry,and coating morphology was observed by scanning electronic microscopy(SEM).Corrosion resistance of the tin coating was analyzed by electrochemical methods.The results indicated that Pb content in the tin coating reduced as bath temperature increased.When the temperature exceeded 40°C,the grains in the coating were coarse and loose,reducing the corrosion resistance.As current density increased,Pb contentincreased rapidly,while low currentdensity plating could lead to drain regions.The plating speed had no obvious effect on trace Pb in tin coating.In the tin plating layer,Pb was enriched at the surface and gradually reduced to zero along the depth.At bath temperature of 40 °C and current density of 20 A·dm-2,the amount of Pb could be less than 100 mg·kg-1 with excellent corrosion resistance.

1.Introduction

Tinplate is widely used in food and beverage packaging due to its non-toxicity,beautifulappearance,corrosion resistance,and other characteristics[1-4].For example,the consumption of tinned steel in above industry is up to 1300 ton·a-1in recentyears.With the developmentof living standards ofpeople,highersafety in food packaging is strongly required.In 2005,EU issued the law of“Steel for packaging — Flat steel products intended for use in contactwith food stuffs,products or beverages for human and animal consumption — Tin coated steel”[5],which demands that trace Pb in tin coating should be less than 0.01%.A new standard is ten times lower than the original standard so that the old tin plating process has to be modi fied as soon as possible.It is known that the tin used in the tinplate usually contains trace Pb,and the standard potential of Sn/Sn2+and Pb/Pb2+is-0.136 V and-0.126 V vs.normal hydrogen electrode,respectively,leading to codeposition easily in electroplating process[6-11].The trace Pb in tin coating often exceeds 100 mg·kg-1,which is unable to meet new environmental requirement.

In tin plating industry,high rate phenol sulfonic acid(PSA)plating[12]is widely applied due to its high ef ficiency,low cost,and highperformance products.Researches have focused on the process of lead-tin alloy plating and effects of parameters and additives on coating quality[13-15],while the trace Pb in tin coating is rarely reported.Therefore,it is urgent to examine the effect of operation parameters in PSA bath plating process on trace Pb.

In this paper,the in fluence of bath temperature,current density and plating speed on trace Pb in tin coating is studied.A briefanalysis on the deposition mechanism of tin plating process and appropriate methods to reduce the Pb content and maintain coating quality is given.

2.Experimental

2.1.Preparation for test

Test substrate is MR low carbon aluminum killed steel.Its ingredients are as follows(mass fraction,%):C 0.12,Mn 0.60,P 0.02,S 0.05,Si 0.02,Cu 0.20.Specimen was cut into rectangular piece(100 mm×60 mm×0.20 mm),with the pretreatment as follows:alkali cleaning(NaOH 15-25 g·L-1;SNN41 2-4 g·L-1;1 min;45 °C)→electrochemical alkali cleaning(NaOH 15-25 g·L-1;SNN41 2-4 g·L-1;5 A·dm-2;2 min;50 °C) → water cleaning(pH ≤ 11;1 min;40 °C) → electrolytic picking(H2SO460-80 g·L-1;3 A·dm-2;2 min;30°C)→ water cleaning(pH ≥3;1 min;35°C).

2.2.Electroplating process conditions

Tin plating was performed in a self-made rotating-cathode plating apparatus.The plating solution is PSA system,with bath condition as follows:Sn2+27 g·L-1,free acid H+16 g·L-1,ENSA 2.8 g·L-1,EN 4.6 g·L-1,Pb 17 mg·L-1,pH 1.0.Bath temperature was set at 35,40,45,and 50 °C;current density was 10,15,20,25,and 30 A·dm-2;plating speed was 80,100,120 and 140 m·min-1.To ensure singleside tin coating weight2.8 g·m-2atleast,the plating time was adjusted appropriately between 2 s and 20 s.

2.3.Characterization tests

Trace Pb in tin coating was detected by atomic absorption spectrometry.The tin coating was firststripped by hydrochloric acid;then,the tin in the solution was removed by hydrobromic acid;graphite furnace atomic absorption(HITACHI,Z2700,Japan)was used to detect trace Pb of stripping solution.The surface morphology of the coating under different processing conditions was observed by scanning electron microscope(JEOL,JSM-6510A,Japan).

In order to examine corrosion behavior of the tinplates,Tafel measurements[16,17]were performed by electrochemical workstation(CorrTest,CS350,China).A three-electrode arrangement was adopted,with the working electrode(1 cm2of exposed area),saturated calomel electrode as the reference electrode,and platinum mesh as the counter electrode.The test solution was 3.5%sodium chloride with scanning rate of 10 mV·s-1and scanning range of-0.4 to-1.2 V.

The distribution of elements Pb,Sn,Fe and O along coating depth in tin coating was determined by glow discharge spectrometer(SPECTRO,GDA750,Germany).

3.Results and Discussion

3.1.Effect of bath temperature on trace Pb in tin coating

Fig.1 illustrates the in fluence of bath temperature on Pb content at current density of 20 A·dm-2and plating speed of 120 m·min-1.Pb content in the tin coating reduces quickly as bath temperature increases.At temperatures higher than 40°C,Pb content is lower than 100 mg·kg-1.

Fig.1.Effect of bath temperature on Pb content in tin coating.

Higher bath temperature is bene ficial to lowering Pb content in tin coating,but introduces adverse effect on corrosion resistance.At high bath temperature,the microstructure of tin coating is loose,as shown in Fig.2.Tin grains are larger.At 40°C,the density of uniform grains of coating is the lowest,suggesting best corrosion resistance.Considering both coating quality and Pb content,the optimal temperature is 40°C.

Fig.3 shows polarization curves of tin coating prepared at different bath temperatures.Fitted corrosion current and potential of each tin coating are list in Table 1.As bath temperature increases from 35°C to 50°C,corrosion current of tin coating reduces first and then increases,while the potential is opposite.It means that the tinplate shows the best corrosion resistance at bath temperature 40°C,consistent with the smallest coating grains in Fig.2.

3.2.Effect of current density on trace Pb

Fig.4 illustrates the in fluence of current density on Pb content in tin coating at bath temperature 20 °C and plating rare 120 m·min-1.Pb content in tin coating increases gradually as current density increases.When the current density is over 25 A·dm-2,Pb content is higher than 100 mg·kg-1,which cannot meet the new standard.

Current density has signi ficant in fluence on the polarization and Pb content in tinplate coating.According to the electrochemical polarization potential and current reaction Butler-Volmer equation[18],

where I is the current density,I0is the exchange current,α is the electron transfer coef ficient,n is the number of electron transferred reaction,F is the Faraday constant,R is the molar gas constant,and T is the bath temperature.In a high-speed tin plating process,bath and cathode plate move relatively and quickly so that exchanged ions can be supplied suf ficiently in time.

Eq.(1)leads to

where η is the electrochemical polarization potential,a and b are the Tafel constants.

According to Eq.(2),in the electrochemical polarization,a linear relation exists between electrode potential and logarithm of current density.Tin plating is essentially an electrocrystallization of metal,including the formation and growth of crystal nucleus[19].The two processes occur simultaneously and their relative rate determines the size of tin grains.When the formation rate of crystal nucleus is higher than the growth rate, fine crystals and dense deposition can be obtained in the plating process.On the contrary,the crystallization becomes coarse.When the cathode current density is small,low cathode polarization formats less crystal nucleus at low rate[20],resulting in larger grains.As the current density increases,the electrochemical overpotential increases.As a result,the number of crystal nuclei increases and the grain size decreases.Nucleation rate is derived by Volmer and Weber[21]:

where v1is the nucleation rate,v2is the crystal growth rate,η is the electrochemical polarization overpotential,and K1and K2are the constants.

Eqs.(3)and(4)show thatthe electrochemicalpolarization increases with the current density.Nucleation rate is much higher than the growth rate,which re fine grains.

Fig.5 shows the surface morphologies of the coating at different current densities.Some leakage areas appear at low cathode current density(Fig.5(a)).As current density increases,the nucleation rate is greatly improved,which lead to grain re finement of electrodeposited tin layer.

Fig.6 shows polarization curves at different current densities.Fitted corrosion currents and potentials are list in Table 2.With the increase of current density,corrosion current of tin coating decreases,the crystallization of tin plating layer tends to be uniform and fine.The corrosion current is gradually reduced and the corrosion resistance is better.Considering both Pb content in coating and corrosion resistance,the current density in PSA should be less than 20 A·dm-2.

Fig.2.Morphology of tin coatings at different bath temperatures.(a)35 °C;(b)40 °C;(c)45 °C;(d)50 °C.

Fig.3.Tafel curves of tin plating at different bath temperatures.

Table 1 Electrochemical corrosion data of tin plating prepared at different bath temperatures

3.3.Effect of plating speed on trace Pb

Fig.7 illustrates the in fluence of plating speed on Pb content at current density 20 A·cm-2and bath temperature 40 °C.The plating speed has little in fluence on trace Pb in tin coating.Itcould be explained as follows:the plating speed is much higher than ion exchange rate,so thatspecimen is always surrounded by fresh bath even atthe minimum speed.Therefore,it is not needed to consider the effect of plating speed in production.

3.4.Distribution of Pb along coating depth in coating

Fig.4.Effect of current density on trace Pb in tin coating.

Fig.5.Scanning electronic microscopy of tin coatings at different current densities.(a)10 A·dm-2;(b)20 A·dm-2;(c)25 A·dm-2;(d)30 A·dm-2.

Fig.6.Tafel curves of tin plating at different current densities.

Fig.8 shows the result of glow discharge spectrometry(GDS)at current density of 20 A·dm-2,bath temperature of 40 °C,and plating speed of 120 m·min-1,with the distribution of Pb,Sn,Fe,and O contents in coating along the depth.The Pb content is relatively high at the coating surface and gradually reduces along the coating depth.Fig.8 could be divided into four parts according to the content of elements Sn and Fe.Parts I,II,III and IV are coating surface layer,pure tin layer,Sn-Fe alloy interlayer,and Fe substrate,respectively.Part I is mainly tin and tin oxide with the thickness of 0.03 μm,enrichment ofPb element.Part II is about 0.23 μm in-depth with a gradual decline of Pb content.In part III,Pb has a peak and then declines,while oxygen has a weak peak.One of possible explanations is that tin reacts with increasing oxygen and tin oxide reduces cathode polarization voltage,reducing Pb deposition in Part III.

Table 2 Electrochemical corrosion data of tin plating at different current densities

4.Conclusions

As bath temperature increases,trace Pb in tin coating reduces quickly;when bath temperature exceeds 40°C,tin grains in coating are coarse and loose,and the corrosion resistance of coating decreases.As current density increases,Pb content increases rapidly,but low current density in plating could lead to drain regions.In high speed plating process in PSA bath,the plating speed has no obvious effect on trace Pb in tin coating.Trace Pb is associated with the tin plating layer,enriched near the surface and gradually reduced to zero along the depth in coating.At bath temperature of 40°C and current density of 20 A·dm-2,Pb content maintains less than 100 mg·kg-1in tinplated coating with excellent corrosion resistance.

Fig.7.Effect of plating speed on trace Pb in tin coating.

Fig.8.Distribution of elements Sn,Fe,O and Pb along tin coating depth by GDS.

主站蜘蛛池模板: 亚洲日韩精品伊甸| 国产激情无码一区二区免费| 一区二区午夜| 国产精品女人呻吟在线观看| 亚洲欧美另类视频| 久久久久青草大香线综合精品| 在线播放精品一区二区啪视频| 成人精品视频一区二区在线| 日韩不卡免费视频| 国产一级无码不卡视频| 思思99思思久久最新精品| a毛片免费看| 精品国产免费第一区二区三区日韩| 国产成人精品在线| 国产经典免费播放视频| 色久综合在线| 欧美日韩国产精品综合| 思思热在线视频精品| 欧美国产精品不卡在线观看| 国产精品永久在线| 一本色道久久88| 自偷自拍三级全三级视频| 日韩a级毛片| 亚洲综合中文字幕国产精品欧美| 国产精品va| 欧美成人手机在线视频| 国产产在线精品亚洲aavv| 日韩无码黄色| 国产黄在线免费观看| 国产无码精品在线播放 | 好吊妞欧美视频免费| 99视频国产精品| 免费毛片视频| 亚洲国产日韩视频观看| 4虎影视国产在线观看精品| 国产美女无遮挡免费视频| WWW丫丫国产成人精品| 亚洲无码视频一区二区三区| 亚洲日韩AV无码精品| 一区二区偷拍美女撒尿视频| 国产精品性| 精品视频福利| 狂欢视频在线观看不卡| 久久精品国产在热久久2019| av一区二区三区在线观看| 五月天久久综合| 乱人伦99久久| 九色视频最新网址| 中文字幕在线免费看| 中文字幕调教一区二区视频| 日韩视频免费| 亚洲AⅤ永久无码精品毛片| 五月婷婷激情四射| 免费aa毛片| 国产成人精品高清在线| 久久精品这里只有精99品| 91丝袜乱伦| 欧美综合成人| 亚洲精品麻豆| 亚洲欧美激情小说另类| 26uuu国产精品视频| 在线欧美日韩| 黄色在线不卡| 欧美午夜在线观看| 日韩在线影院| 国产香蕉在线视频| 91啪在线| 91精品国产91久久久久久三级| 美女视频黄又黄又免费高清| 刘亦菲一区二区在线观看| 99视频国产精品| 尤物特级无码毛片免费| 国产成人久久综合777777麻豆| 国产呦精品一区二区三区网站| 自拍亚洲欧美精品| AV片亚洲国产男人的天堂| 亚洲午夜福利精品无码| 欧美成人看片一区二区三区| 人人爱天天做夜夜爽| 一边摸一边做爽的视频17国产| 欧美 国产 人人视频| 一级毛片在线播放|